NIST High Temp. Superconducting Materials (HTS) Database:

NIST Standard Reference Database 62

Last Update to Data Content: 1996

DOI: https://doi.org/10.18434/T4KP8J


Bibliographic Information

Title: Low-Temperature Crystal Structure and Superconductivity in La2-xBaxCuO4
Author(s): N. Momono, M. Ido, M. Oda, N. Yamada, A. Onodera, Y. Okajima, and K. Yamaya
Publication: Physica C Volume: 183 Issue: Not Available Year: 1991 Page(s): 241-246
Editor(s): Not Available
Publisher: Elsevier Science Publishers B.V.
Language: English
Notes: Not Available
Keywords: Material Specification, Magnetic Susceptibility, Thermal Expansion

Materials and Properties

La:21; [La(Ba)-Cu-O]
Material Specification for La:21; [La(Ba)-Cu-O] Process: Solid State Reaction
Notes: "The La2-xBaxCuOx crystals were prepared by firing La2O3, BaCO3 and CuO. The well-mixed powders fired at 1060 °C in flowing oxygen for 24 h and slowly cooled at a rate 1.5 °C/min."
Formula: La2-xBaxCuO4
Informal Name: La:21
Chemical Family: La(Ba)-Cu-O
Chemical Class: Oxide
Structure Type: Polycrystalline
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:

Magnetic Susceptibility for La:21; [La(Ba)-Cu-O]
x of Bax (formula units) Temperature (K) Magnetic Susceptibility (arbitrary)
0.125 2 -0.65
0.125 6 -0.41
0.125 11 -0.25
0.125 16 -0.18
0.125 20 -0.10
0.125 23 -0.02
0.125 28 0.00
0.102 10 -8.71
0.102 13 -8.71
0.102 16 -8.15
0.102 21 -4.90
0.102 25 -1.73
0.102 27 -0.60
0.102 29 -0.03
0.102 31 0.00
0.09 13 -9.10
0.09 16 -9.10
0.09 19 -8.86
0.09 22 -8.13
0.09 25 -6.26
0.09 28 -2.44
0.09 29 -1.14
0.09 30 -0.32
0.09 31 0.00
Measurement Method: SQUID magnetometer
"The diamagnetic susceptibility of the superconductivity was measured by a SQUID susceptometer. The measurements were carried out at a field of (1.2 kA/m = 15 Oe)."

Cautions: Evaluated Data
Digitized data were obtained from Figure 7 of the paper.
Thermal Expansion for La:21; [La(Ba)-Cu-O]
x of Bax (formula units) Temperature (K) Thermal Expansion (10-6 K-1)
0.096 24 1.3
0.096 32 2.0
0.096 46 3.4
0.096 78 5.4
0.096 107 7.2
0.096 139 8.1
0.096 172 9.2
0.096 196 9.8
0.104 20 3.0
0.104 38 3.9
0.104 50 5.2
0.104 80 7.7
0.104 109 8.8
0.104 141 10.3
0.104 175 11.3
0.104 196 11.7
0.125 21 2.2
0.125 41 3.6
0.125 56 4.8
0.125 65 7.0
0.125 83 8.6
0.125 113 10.3
0.125 146 11.9
0.125 179 13.0
0.125 204 13.9
Measurement Method: Thermal expansion method
"The thermal expansion coefficient was measured by means of the strain gage method, where Cu of high purity was used as a reference material." No additional measurement details were noted.

Cautions: Evaluated Data
Digitized data were obtained from Figure 6 of the paper.