Material Specification for Tm:123; [Tm-Ba-Cu-O]
Process: Crystal Growth
Notes: "We present the temperature dependences of the thermal conductivity... of single crystalline Bi2Sr2CaCu2Ox and TmBa2Cu3Ox." No additional sample preparation or characterization information was noted.
Formula: TmBa2Cu3Ox
Informal Name: Tm:123
Chemical Family: Tm-Ba-Cu-O
Chemical Class: Oxide
Structure Type:
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Critical Temperature for Tm:123; [Tm-Ba-Cu-O]
Critical Temperature (K) |
90 |
Measurement Method: Four-point transport method
The authors cite F.G. Aliev, et al., Sov. J. Superconduct. (Russ. Ed.), Vol. 3, 348 (1990), and summarize the procedure as follows. "... transport properties were measured... on single crystals with an average dimension of about (3*1*0.1)mm
3, by means of an electrical, dc and thermal, constant gradient, four-point method."
Cautions: Evaluated Data
Resistivity (normal state) for Tm:123; [Tm-Ba-Cu-O]
Temperature (K) |
Resistivity (normal state) (mΩ·cm) |
89 |
0.02 |
90 |
0.11 |
95 |
0.21 |
100 |
0.23 |
120 |
0.45 |
Measurement Method: Four-point transport method
The authors cite F.G. Aliev, et al., Sov. J. Superconduct. (Russ. Ed.), Vol. 3, 348 (1990), and summarize the procedure as follows. "... transport properties were measured... on single crystals with an average dimension of about (3*1*0.1)mm
3, by means of an electrical, dc and thermal, constant gradient, four-point method."
Cautions: Evaluated Data
Digitized data were obtained from Fig. 1 of the paper.
Thermal Conductivity for Tm:123; [Tm-Ba-Cu-O]
Temperature (K) |
Thermal Conductivity (W m-1 K-1) |
12 |
4.2 |
24 |
6.0 |
41 |
7.1 |
56 |
7.7 |
83 |
7.0 |
97 |
6.6 |
125 |
6.7 |
Measurement Method: Four-point transport method
The authors cite F.G. Aliev, et al., Sov. J. Superconduct. (Russ. Ed.), Vol. 3, 348 (1990), and summarize the procedure as follows. "... transport properties were measured... on single crystals with an average dimension of about (3*1*0.1)mm
3, by means of an electrical, dc and thermal, constant gradient, four-point method."
Cautions: Evaluated Data
Digitized data were obtained from Figure 1 of the paper.
=
Material Specification for Bi:2212; [Bi-Sr-Ca-Cu-O]
Process: Solid State Reaction
Notes: "We present the temperature dependences of the thermal conductivity... of single crystalline Bi2Sr2CaCu2Ox and TmBa2Cu3Ox." No additional sample preparation or characterization information was noted.
Formula: Bi2Sr2CaCu2Ox
Informal Name: Bi:2212
Chemical Family: Bi-Sr-Ca-Cu-O
Chemical Class: Oxide
Structure Type: Polycrystalline
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Thermal Conductivity for Bi:2212; [Bi-Sr-Ca-Cu-O]
Temperature (K) |
Thermal Conductivity (W m-1 K-1) |
81 |
4.7 |
93 |
4.5 |
106 |
4.4 |
115 |
4.2 |
121 |
4.5 |
132 |
4.6 |
Measurement Method: Four-point transport method
The authors cite F.G. Aliev, et al., Sov. J. Superconduct. (Russ. Ed.), Vol. 3, 348 (1990), and summarize the procedure as follows. "... transport properties were measured... on single crystals with an average dimension of about (3*1*0.1)mm
3, by means of an electrical, dc and thermal, constant gradient, four-point method."
Cautions: Evaluated Data
Digitized data were obtained from Figure 2 of the paper.