Film Thickness () | Field Direction () | Temperature (K) | Irreversibility Field (T) |
6000 | //c-axis | 76.3 | 9.0 |
6000 | //c-axis | 78.7 | 7.0 |
6000 | //c-axis | 81.1 | 5.0 |
6000 | //c-axis | 83.8 | 3.0 |
6000 | //c-axis | 86.6 | 1.4 |
6000 | //c-axis | 88.7 | 0.4 |
6000 | //c-axis | 89.8 | 0 |
6000 | //ab-plane | 86.3 | 9.0 |
6000 | //ab-plane | 87.1 | 7.0 |
6000 | //ab-plane | 88.6 | 2.8 |
6000 | //ab-plane | 89.7 | 0.6 |
6000 | //ab-plane | 90.2 | 0 |
250 | //c-axis | 70.2 | 9.0 |
250 | //c-axis | 73.3 | 7.0 |
250 | //c-axis | 76.6 | 5.0 |
250 | //c-axis | 80.6 | 3.0 |
250 | //c-axis | 84.8 | 1.0 |
250 | //c-axis | 86.4 | 0.4 |
250 | //c-axis | 88.1 | 0 |
250 | //c-axis | 88.8 | 0 |
250 | //ab-plane | 85.7 | 9.0 |
250 | //ab-plane | 86.5 | 7.0 |
250 | //ab-plane | 87.3 | 4.4 |
250 | //ab-plane | 87.6 | 4.0 |
250 | //ab-plane | 88.3 | 2.3 |
250 | //ab-plane | 89.0 | 0.9 |
250 | //ab-plane | 89.2 | 0 |