Material Specification for Y:123; [Y-Ba-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: YBa2Cu3O7
Informal Name: Y:123
Chemical Family: Y-Ba-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for Y:123; [Y-Ba-Cu-O]
Temperature (°C) |
Hardness (GPa) |
87 |
13.0 |
110 |
12.5 |
150 |
12.7 |
187 |
11.7 |
226 |
11.0 |
259 |
10.3 |
293 |
10.0 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Digitized data were obtained from Figure 6 of the paper.
Material Specification for Y:123; [Y-Ba-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: YBa2Cu3O6
Informal Name: Y:123
Chemical Family: Y-Ba-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for Y:123; [Y-Ba-Cu-O]
Temperature (°C) |
Hardness (GPa) |
192 |
12.0 |
210 |
11.0 |
240 |
9.4 |
260 |
8.0 |
299 |
7.0 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Digitized data were obtained from Figure 6 of the paper.
Material Specification for La:21; [La-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: La2CuO4
Informal Name: La:21
Chemical Family: La-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for La:21; [La-Cu-O]
Temperature (°C) |
Hardness (GPa) |
85 |
10.2 |
108 |
10.2 |
135 |
9.6 |
166 |
9.1 |
197 |
8.6 |
209 |
8.1 |
226 |
7.7 |
247 |
7.6 |
274 |
7.4 |
293 |
7.5 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Digitized data were obtained from Figure 6 of the paper.
Material Specification for La:21; [La(Sr)-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: La2-xSrxCuO4
Informal Name: La:21
Chemical Family: La(Sr)-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for La:21; [La(Sr)-Cu-O]
Temperature (°C) |
Hardness (GPa) |
83 |
11.1 |
84 |
11.7 |
109 |
11.0 |
110 |
10.6 |
136 |
11.1 |
140 |
10.9 |
161 |
10.6 |
167 |
10.3 |
188 |
10.3 |
192 |
10.0 |
200 |
10.1 |
207 |
10.0 |
217 |
9.3 |
230 |
9.9 |
233 |
9.6 |
265 |
9.3 |
292 |
9.0 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Digitized data were obtained from Figure 6 of the paper.
Material Specification for TlBa:1212; [Tl-Ba-Ca-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: TlBa2CaCu2Ox
Informal Name: TlBa:1212
Chemical Family: Tl-Ba-Ca-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for TlBa:1212; [Tl-Ba-Ca-Cu-O]
Temperature (°C) |
Hardness (GPa) |
300 |
6.8 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Material Specification for Tl:2212; [Tl-Ba-Ca-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: Tl2Ba2CaCu2Ox
Informal Name: Tl:2212
Chemical Family: Tl-Ba-Ca-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for Tl:2212; [Tl-Ba-Ca-Cu-O]
Temperature (°C) |
Hardness (GPa) |
300 |
2.8 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Material Specification for Ho:123; [Ho-Ba-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: HoBa2Cu3Ox
Informal Name: Ho:123
Chemical Family: Ho-Ba-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for Ho:123; [Ho-Ba-Cu-O]
Temperature (°C) |
Hardness (GPa) |
300 |
5.9 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Material Specification for Dy:123; [Dy-Ba-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: DyBa2Cu3Ox
Informal Name: Dy:123
Chemical Family: Dy-Ba-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for Dy:123; [Dy-Ba-Cu-O]
Temperature (°C) |
Hardness (GPa) |
300 |
5.7 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data
Material Specification for Yb:123; [Yb-Ba-Cu-O]
Process: Solid State Reaction
Notes: All materials were single crystals. No additional processing details were noted.
Formula: YbBa2Cu3Ox
Informal Name: Yb:123
Chemical Family: Yb-Ba-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Hardness for Yb:123; [Yb-Ba-Cu-O]
Temperature (°C) |
Hardness (GPa) |
300 |
5.1 |
Measurement Method: Vickers indentation
The author cites L. S. Fomenko et al., Superconductivity: Phys. Chem. Tech., Vol. 4, 2394 (1991) [in Russian], and summarizes the procedure by noting that the Vickers microhardness of single crystals was determined with a load of 0.15 N.
Cautions: Evaluated Data