Material Specification for Tl:1223; [Tl-Ba-Ca-Cu-O]
Process: Melt Processed
Notes: The authors cite A. Maignan et al., Physica C, Vol. 219, 407 (1994), and summarize the procedure as follows. "Single crystals have been grown from melts of BaCuO2:CaO:Tl2O3 in the ratio 2:2:1/2. ... One of these crystals, with dimensions 0.81 x 0.48 x 0.13 mm3, was retained for the magnetic study."
Formula: TlBa2Ca2Cu3O9
Informal Name: Tl:1223
Chemical Family: Tl-Ba-Ca-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer: In House
Commercial Name: In House
Production Date:
Lot Number:
Production Form:
Critical Temperature for Tl:1223; [Tl-Ba-Ca-Cu-O]
Critical Temperature (K) |
114 |
Measurement Method: SQUID magnetometer
"...J
c values and the irreversibility line location derived from magnetic hysteresis loops are presented... The magnetic measurements were carried out by means of a 5.5 T SQUID magnetometer in the configuration H//c. ... The critical current densities have been evaluated from the hysteresis loops using an extended Bean model for rectangular shaped samples. ... For temperatures not too close to T
c ( ≤ 105 K), the determination of H
(T) using the closing points of the hysteresis loops is quite definite."
Cautions: Evaluated Data
Critical Current Density for Tl:1223; [Tl-Ba-Ca-Cu-O]
Temperature (K) |
Magnetic Field (kA/m) |
Critical Current Density (kA/cm2) |
30 |
850 |
720 |
30 |
1400 |
600 |
30 |
2400 |
430 |
40 |
83 |
310 |
40 |
230 |
260 |
40 |
490 |
290 |
40 |
1000 |
280 |
40 |
2000 |
150 |
40 |
3800 |
50 |
50 |
120 |
140 |
50 |
230 |
160 |
50 |
490 |
180 |
50 |
1000 |
110 |
50 |
1800 |
38 |
50 |
2600 |
15 |
50 |
4000 |
3.6 |
60 |
47 |
80 |
60 |
160 |
89 |
60 |
400 |
100 |
60 |
1000 |
33 |
60 |
1600 |
7.0 |
60 |
2300 |
1.5 |
60 |
2700 |
0.23 |
60 |
3500 |
0.037 |
70 |
39 |
32 |
70 |
170 |
48 |
70 |
330 |
47 |
70 |
650 |
16 |
70 |
990 |
3.3 |
70 |
1300 |
0.38 |
70 |
1600 |
0.051 |
80 |
24 |
15 |
80 |
39 |
13 |
80 |
76 |
15 |
80 |
150 |
22 |
80 |
260 |
19 |
80 |
400 |
8.6 |
80 |
500 |
2.5 |
80 |
680 |
0.62 |
80 |
810 |
0.18 |
90 |
15 |
6.2 |
90 |
32 |
3.8 |
90 |
67 |
5.8 |
90 |
120 |
9.0 |
90 |
200 |
4.1 |
90 |
290 |
1.2 |
90 |
460 |
0.034 |
100 |
6 |
4.0 |
100 |
16 |
1.3 |
100 |
49 |
0.80 |
100 |
59 |
0.58 |
100 |
110 |
0.57 |
100 |
140 |
0.089 |
100 |
160 |
0.022 |
100 |
160 |
0.140 |
100 |
180 |
0.0048 |
100 |
180 |
0.041 |
100 |
190 |
0.019 |
100 |
210 |
0.0088 |
Measurement Method: SQUID magnetometer
"...J
c values and the irreversibility line location derived from magnetic hysteresis loops are presented... The magnetic measurements were carried out by means of a 5.5 T SQUID magnetometer in the configuration H//c. ... The critical current densities have been evaluated from the hysteresis loops using an extended Bean model for rectangular shaped samples. ... For temperatures not too close to T
c ( ≤ 105 K), the determination of H
(T) using the closing points of the hysteresis loops is quite definite."
Cautions: Evaluated Data
Digitized data were obtained from Figure 4 of the paper.
Irreversibility Field for Tl:1223; [Tl-Ba-Ca-Cu-O]
Temperature (K) |
Irreversibility Field (T) |
60 |
4.0 |
70 |
2.0 |
80 |
1.1 |
90 |
0.56 |
100 |
0.27 |
105 |
0.12 |
107 |
0.087 |
Measurement Method: SQUID magnetometer
"...J
c values and the irreversibility line location derived from magnetic hysteresis loops are presented... The magnetic measurements were carried out by means of a 5.5 T SQUID magnetometer in the configuration H//c. ... The critical current densities have been evaluated from the hysteresis loops using an extended Bean model for rectangular shaped samples. ... For temperatures not too close to T
c ( ≤ 105 K), the determination of H
(T) using the closing points of the hysteresis loops is quite definite."
Cautions: Evaluated Data
Digitized data were obtained from Figure 6 of the paper.