NIST High Temp. Superconducting Materials (HTS) Database:

NIST Standard Reference Database 62

Last Update to Data Content: 1996

DOI: https://doi.org/10.18434/T4KP8J


Bibliographic Information

Title: Susceptibility measurement by SQUID
Author(s): Not Available
Publication: STA Project Data Volume: Not Available Issue: Not Available Year: 1993 Page(s): Not Available
Editor(s): Not Available
Publisher: Science and Technology Agency of Japan
Language: Japanese
Notes: STA sheet number: 6268,6269
Keywords: Material Specification, Magnetic Susceptibility

Materials and Properties

Y:123; [Y-Ba-Cu-O]
Material Specification for Y:123; [Y-Ba-Cu-O] Process:
Notes:
Formula: YBa2Cu3Oz
Informal Name: Y:123
Chemical Family: Y-Ba-Cu-O
Chemical Class: Oxide
Structure Type: Single Crystal
Manufacturer:
Commercial Name:
Production Date:
Lot Number: YBCO
Production Form:
Magnetic Susceptibility for Y:123; [Y-Ba-Cu-O]
Field Condition () Temperature (K) Magnetic Susceptibility (arbitrary)
H//a,b 5.66 -0.0196
H//a,b 10.4 -0.0196
H//a,b 20.3 -0.0198
H//a,b 29.6 -0.0197
H//a,b 40.5 -0.0195
H//a,b 50.2 -0.0197
H//a,b 56.3 -0.0196
H//a,b 59.8 -0.0195
H//a,b 65.5 -0.0197
H//a,b 68 -0.0197
H//a,b 70.1 -0.0196
H//a,b 72.9 -0.0197
H//a,b 75.1 -0.0197
H//a,b 77.8 -0.0197
H//a,b 79.2 -0.0197
H//a,b 81.1 -0.0197
H//a,b 82.2 -0.0197
H//a,b 83.2 -0.0197
H//a,b 84 -0.0197
H//a,b 84.7 -0.0197
H//a,b 85.9 -0.0197
H//a,b 86.7 -0.0197
H//a,b 87.1 -0.0197
H//a,b 88.5 -0.0196
H//a,b 89.1 -0.0194
H//a,b 90.1 -0.0171
H//a,b 91.1 -0.00763
H//a,b 5.66 0.00105
H//a,b 10.1 0.00106
H//a,b 20.2 0.00109
H//a,b 30.3 0.00109
H//a,b 40.3 0.000978
H//a,b 46 0.00101
H//a,b 50 0.000985
H//a,b 54.8 0.000939
H//a,b 60 0.000943
H//a,b 62.6 0.000994
H//a,b 65 0.000921
H//a,b 67.6 0.000973
H//a,b 70.4 0.00102
H//a,b 72.5 0.001
H//a,b 74.6 0.000953
H//a,b 75.7 0.00088
H//a,b 76.3 0.000905
H//a,b 77.6 0.00098
H//a,b 77.9 0.000956
H//a,b 78.2 0.000956
H//a,b 79.1 0.000957
H//a,b 79.7 0.00106
H//a,b 80.8 0.00106
H//a,b 81.9 0.000983
H//a,b 82.8 0.000984
H//a,b 84.4 0.00106
H//a,b 85.1 0.000961
H//a,b 85.7 0.000961
H//a,b 86.5 0.000937
H//a,b 87.1 0.000938
H//a,b 87.8 0.00101
H//a,b 88.5 0.00101
H//a,b 89.8 0.00111
H//a,b 90.4 0.00106
H//a,b 92.1 -0.000446
H//a,b 92.6 -0.000297
H//a,b 94.5 -0.000221
H//a,b 96.4 -0.000195
H//a,b 98.7 -0.000193
H//a,b 101 -0.0000928
H//a,b 103 -0.000141
H//a,b 105 -0.00014
H//a,b 107 -0.000138
H//a,b 110 -0.000136
H//a,b 113 -0.000084
H//a,b 115 -0.0000826
H//a,b 117 -0.000131
H//a,b 120 -0.000203
H//a,b 125 -0.000199
H//a,b 130 -0.0000959
H//a,b 135 0.00000661
H//a,b 140 -0.000164
H//a,b 146 -0.0000845
H//a,b 150 -0.000156
H//c 5.64 -0.0257
H//c 10.1 -0.0258
H//c 20.4 -0.0255
H//c 30 -0.0256
H//c 39.7 -0.0257
H//c 50.3 -0.0257
H//c 55.3 -0.0256
H//c 59.5 -0.0256
H//c 66 -0.0257
H//c 67.3 -0.0258
H//c 70.6 -0.0256
H//c 72 -0.0256
H//c 75.2 -0.0257
H//c 77.5 -0.0257
H//c 79.3 -0.0257
H//c 79.9 -0.0257
H//c 80.5 -0.0258
H//c 81.2 -0.0257
H//c 82.1 -0.0256
H//c 83 -0.0257
H//c 84.6 -0.0256
H//c 85 -0.0256
H//c 86 -0.0257
H//c 87 -0.0256
H//c 87.3 -0.0256
H//c 88.3 -0.0256
H//c 90.2 -0.0253
H//c 91.5 -0.0153
H//c 92.6 -0.0029
H//c 5.18 0.0015
H//c 10.8 0.00167
H//c 20.8 0.00163
H//c 29.8 0.00161
H//c 39.7 0.00157
H//c 44.2 0.00153
H//c 49.2 0.00153
H//c 55.2 0.00161
H//c 60.2 0.00154
H//c 62.4 0.00161
H//c 64.7 0.00154
H//c 67.4 0.00149
H//c 70.4 0.00155
H//c 72.9 0.00155
H//c 75.4 0.00155
H//c 76.9 0.00133
H//c 77.4 0.00145
H//c 78.5 0.00145
H//c 79.2 0.00143
H//c 79.8 0.00148
H//c 81.4 0.00138
H//c 82.1 0.00141
H//c 83 0.00143
H//c 84.7 0.00143
H//c 85.9 0.00153
H//c 86.7 0.00151
H//c 87.9 0.00153
H//c 88.3 0.00153
H//c 89.3 0.00161
H//c 90.5 0.00163
H//c 91.8 0.00168
H//c 92.2 0.000248
H//c 93.2 -0.000272
H//c 94.7 -0.000221
H//c 95.8 -0.000245
H//c 96.2 -0.000146
H//c 96.4 -0.00022
H//c 97.2 -0.00012
H//c 98.7 -0.000144
H//c 100 -0.0000684
H//c 101 -0.000192
H//c 103 -0.0000915
H//c 104 -0.00019
H//c 107 -0.000138
H//c 109 -0.0000617
H//c 112 -0.000109
H//c 115 -0.0000821
H//c 118 -0.00013
H//c 120 -0.000103
H//c 125 -0.000248
H//c 130 -0.000171
H//c 135 -0.0000183
H//c 140 -0.0000392
H//c 145 -0.00011
H//c 150 -0.000106
Measurement Method: Susceptibility (SQUID)
Test facility: Faculty of Science, Hiroshima University Location: Cryogenics Center, Hiroshima University Test date: 1989/1/28 Environment temperature: 20 °C Laboratory environment: air conditioned Test atmosphere: He gas Applied pressure: 105 Pa SQUID scanning width: 40 mm Temperature control: gas cooling Test temperature: 5 K - 150 K Applied field (1): 0.2 mT Field direction (1): field cooling, H//ab Applied field (2): 0.2 mT Field direction (2): field cooling, H//c Data comment: no diamagnetism modification Test equipment: SQUID Maker of test equipment: QD Model of test equipment: MPMS Other test equipment: 92SIS69Y Specimen treatment: no special Specimen holding: being fixed on straw

Cautions: Research Data