NIST High Temp. Superconducting Materials (HTS) Database:

NIST Standard Reference Database 62

Last Update to Data Content: 1996

DOI: https://doi.org/10.18434/T4KP8J


Bibliographic Information

Title: Dependence of thermal conductivity on temperature for Ag sheathed Bi2Sr2CaCu2Ox tape
Author(s): Not Available
Publication: STA Project Data Volume: Not Available Issue: Not Available Year: 1993 Page(s): Not Available
Editor(s): Not Available
Publisher: Science and Technology Agency of Japan
Language: Japanese
Notes: STA sheet number: 6275,6277
Keywords: Material Specification, Thermal Conductivity

Materials and Properties

Bi:2212; [Bi-Sr-Ca-Cu-O]
Material Specification for Bi:2212; [Bi-Sr-Ca-Cu-O] Process:
Notes:
Formula: Bi2Sr2CaCu2O8
Informal Name: Bi:2212
Chemical Family: Bi-Sr-Ca-Cu-O
Chemical Class: Oxide
Structure Type:
Manufacturer:
Commercial Name:
Production Date:
Lot Number: 92AAGBLA-29
Production Form:
Thermal Conductivity for Bi:2212; [Bi-Sr-Ca-Cu-O]
Tc(end) (K) Temperature (K) Thermal Conductivity (W m-1 K-1)
92.6 13.3 41.9
92.6 13.3 42.0
92.6 13.3 43.2
92.6 17.2 47.1
92.6 17.2 48.5
92.6 17.2 46.1
92.6 22.1 48.9
92.6 22.1 49.2
92.6 22.1 49.2
92.6 26.9 46.3
92.6 26.9 47.1
92.6 26.9 46.9
92.6 32.2 41.0
92.6 32.2 40.8
92.6 32.2 42.0
92.6 37.2 36.6
92.6 37.2 36.3
92.6 37.2 36.1
92.6 42.5 32.6
92.6 42.5 32.4
92.6 42.5 32.7
92.6 47.5 30.2
92.6 47.5 30.1
92.6 47.5 30.4
92.6 52.5 28.5
92.6 52.5 28.6
92.6 52.5 28.4
92.6 57.7 27.1
92.6 57.7 27.3
92.6 57.7 27.4
92.6 62.8 26.6
92.6 62.7 26.7
92.6 62.8 27.0
92.6 67.9 26.6
92.6 67.9 26.7
92.6 67.9 26.7
92.6 72.9 26.4
92.6 72.9 26.7
92.6 72.9 26.7
92.6 77.9 26.8
92.6 77.9 26.7
92.6 77.9 26.8
92.6 82.9 26.3
92.6 82.9 26.5
92.6 82.9 26.5
92.6 87.9 26.4
92.6 87.9 26.5
92.6 87.9 26.5
92.6 92.9 26.5
92.6 92.9 26.5
92.6 92.9 26.5
92.6 97.9 26.8
92.6 97.9 26.8
92.6 97.9 26.8
92.6 103.0 26.5
92.6 103.0 26.8
92.6 103.0 26.7
92.6 108.3 26.1
92.6 108.3 26.0
92.6 108.3 26.1
92.6 113.3 26.7
92.6 113.3 26.6
92.6 113.3 26.7
92.6 118.3 26.3
92.6 118.3 26.4
92.6 118.3 26.5
92.6 123.4 26.5
92.6 123.4 26.6
92.6 123.4 26.4
92.6 128.5 26.2
92.6 128.5 26.3
92.6 128.5 26.4
92.6 133.5 26.5
92.6 133.5 26.5
92.6 133.5 26.5
92.6 138.5 26.8
92.6 138.5 26.8
92.6 138.5 26.7
92.6 143.5 27.5
92.6 143.5 27.4
92.6 143.5 27.3
Measurement Method: Heat-flux
Test facility: Faculty of Engineering, Iwate University Location: Lab. of Material Property, Iwate University Start date: 1989/2/9 End date: 1989/2/10 Environment temperature: 20 °C Environment humidity: 60 % Test temperature: room temperature Applied pressure: 0.27 mPa (2x10-6 Torr) Remark on test condition: taking a chamber with room temperature and vacuum (about 0.27 mPa) as adiabatic space, cooling the sample stage to the start temperature, adusting sample temperature with a heater Test equipment (1): helium freezer Maker of test equipment (1): Sumitomo Zyuki Model of test equipment (1): SRD204 Test equipment (2): NEC PC-9801RX personal computer Test equipment (3): digital multimeter Maker of test equipment (3): Yokogawa Model of test equipment (3): 2501A Test equipment (4): program power source Maker of test equipment (4): Keithley Model of test equipment (4): Model220 Test equipment (5): scanner Maker of test equipment (5): Advantest Model of test equipment (5): TR7200 Test equipment (6): CGR resistance thermometer Test equipment (7): Au + 0.07 % Fe-Cr thermocouple Remark on test equipments: using a personal computer to realize the automatic measurement Specimen length: 22.3 mm Specimen width: 4.9 mm Specimen thickness: 0.41 mm Distance between specimen and thermometer: 7.75 mm Specimen reinforcement: using a brass plate to reinforce the specimen, size of the plate: 4.9 mm (width), 0.282 mm (thickness) Width of Ag sheathed: 4.9 mm Thickness of Ag sheath: 0.06 mm Width of superconductor: 3 mm Thickness of superconductor: 0.02 mm Remark on specimen: fixing sample by using In and ceramic solder, attaching a thermocouple on the sample by using insulation varnish (GE7031). Data comment: saving the test result in a floppy disk, and printing it out after the test is over Data comment: including the cross section area of Ag sheath when calculating the thermal conductivity at Tc=92.6K

Cautions: Research Data