"Microstructure and Properties of Sintered Silicon Carbides Fabricated by Different Methods," T. Maruyama, H. Kitamura, and T. Iseki, Journal of the Ceramic Society of Japan, Vol. 94 [8], pp. 790-794 (1986), published by Ceramic Society of Japan.Language: Japanese
Material #1, Phases: 73% α(6H); 11% β(3C); 7% α(15R); 9% free Si. Material #2, Phases: 84% α(6H); 7.5% α(4H); 6% α(15R). Material #3, Phases: 87% α(6H); 7.5% α(4H); 5% α(15R); small amount of BeO.
The measurements were made by four-point bend method, inner-span = 10 mm, outer span = 20 mm, crosshead speed = 0.5 mm/min.Scanning electron microscopy (SEM)
The grain size was determined using SEM microscopy.
| Amount of Element ( formula units ) |
Element ( no unit ) |
|---|---|
| 1 | Si |
| 1 | C |
| Density ( g cm-3 ) |
|---|
| 3.12 |
No measurement details were noted.
| Temperature ( °C ) |
Flexural Strength ( MPa ) |
|---|---|
| 22 | 550 |
| Grain Size ( µm ) |
|---|
| 8 |
| Amount of Element ( formula units ) |
Element ( no unit ) |
|---|---|
| 1 | Si |
| 1 | C |
| Density ( g cm-3 ) |
|---|
| 3.13 |
| Temperature ( °C ) |
Flexural Strength ( MPa ) |
|---|---|
| 22 | 470 |
| Grain Size ( µm ) |
|---|
| 5 |
| Amount of Element ( formula units ) |
Element ( no unit ) |
|---|---|
| 1 | Si |
| 1 | C |
| Density ( g cm-3 ) |
|---|
| 3.20 |
| Temperature ( °C ) |
Flexural Strength ( MPa ) |
|---|---|
| 22 | 380 |
| Grain Size ( µm ) |
|---|
| 9 |