NIST Standard Reference Database 30
Last Update to Data Content: 2002
"Elastic Properties of Polycrystalline Monoclinic Sm2O3," O. Hunter, H.J. Korklan, and R.R. Suchomel, Journal of the American Ceramic Society, Vol. 57 [6], pp. 267-268 (1974), published by American Ceramic Society.Language: English
The authors cite J.A. Haglund et al., Journal of the American Ceramic Society, Vol. 56, No. 6, 327 (1973), and summarize the procedure as follows. "The Sm2O3 was produced from zeonotine ore by ion exhange, formation of the oxyacid salt, and calcination to yield the oxide."
The authors cite S. Spinner et al., American Society for Testing and Materials Proceedings, Vol. 61, 1221 (1961), and summarize the procedure as follows. "Elastic properties were measured by the sonic resonance technique. ... High-temperature measurements were made in a vacuum carbon-rod resistance furnace. ... Volume-fraction porosity is based on a theoretical density of 7.748 g/cm3..."
| Volume Fraction of Porosity | Temperature ( °C ) | Elastic Modulus ( GPa ) |
|---|---|---|
| 0.016 | 23 | 138.0 |
| 0.045 | 23 | 131.3 |
| 0.054 | 23 | 131.2 |
| 0.079 | 23 | 120.7 |
| 0.092 | 23 | 121.8 |
| 0.107 | 23 | 111.4 |
| 0.119 | 23 | 110.0 |
| 0.260 | 23 | 64.8 |
| 0.279 | 23 | 62.1 |
| 0.372 | 23 | 39.2 |
| 0.372 | 23 | 36.7 |
| 0.376 | 23 | 35.4 |
| 0.376 | 23 | 32.8 |
| 0.019 | 26 | 137.6 |
| 0.019 | 101 | 135.5 |
| 0.019 | 176 | 133.5 |
| 0.019 | 270 | 132.0 |
| 0.019 | 364 | 129.1 |
| 0.019 | 457 | 126.7 |
| 0.019 | 551 | 125.1 |
| 0.019 | 582 | 123.9 |
| 0.019 | 639 | 123.1 |
| 0.019 | 720 | 121.5 |
| 0.019 | 813 | 119.5 |
| 0.019 | 907 | 117.1 |
| 0.019 | 1001 | 114.7 |
| 0.019 | 1101 | 112.3 |
| 0.019 | 1214 | 109.5 |
| 0.019 | 1314 | 105.5 |
Data were digitized from Figs. 1 and 2 of the reference.
| Volume Fraction of Porosity | Temperature ( °C ) | Gruneisen Parameter ( no unit ) |
|---|---|---|
| 0.019 | 102 | 1.27 |
| 0.019 | 204 | 1.21 |
| 0.019 | 301 | 1.17 |
| 0.019 | 405 | 1.16 |
| 0.019 | 506 | 1.13 |
| 0.019 | 603 | 1.11 |
| 0.019 | 704 | 1.08 |
| 0.019 | 805 | 1.04 |
| 0.019 | 906 | 1.02 |
| 0.019 | 1003 | 1.00 |
| 0.019 | 1107 | 0.98 |
| 0.019 | 1208 | 0.95 |
| 0.019 | 1309 | 0.93 |
| 0.019 | 1406 | 0.91 |
Data were digitized from Fig. 2 of the reference.
| Volume Fraction of Porosity | Temperature ( °C ) | Poisson's Ratio ( no unit ) |
|---|---|---|
| 0.019 | 23 | 0.322 |
| 0.023 | 23 | 0.319 |
| 0.048 | 23 | 0.326 |
| 0.053 | 23 | 0.328 |
| 0.082 | 23 | 0.312 |
| 0.092 | 23 | 0.332 |
| 0.108 | 23 | 0.304 |
| 0.116 | 23 | 0.319 |
| 0.265 | 23 | 0.261 |
| 0.278 | 23 | 0.253 |
| 0.372 | 23 | 0.250 |
| 0.373 | 23 | 0.242 |
| 0.377 | 23 | 0.240 |
| 0.373 | 23 | 0.235 |
Data were digitized from Fig. 1 of the reference.
| Volume Fraction of Porosity | Temperature ( °C ) | Shear Modulus ( GPa ) |
|---|---|---|
| 0.017 | 23 | 52.1 |
| 0.023 | 23 | 52.1 |
| 0.047 | 23 | 50.5 |
| 0.055 | 23 | 50.4 |
| 0.082 | 23 | 46.3 |
| 0.093 | 23 | 46.2 |
| 0.108 | 23 | 42.1 |
| 0.118 | 23 | 40.8 |
| 0.263 | 23 | 26.3 |
| 0.278 | 23 | 24.9 |
| 0.373 | 23 | 16.2 |
| 0.377 | 23 | 13.6 |
| 0.019 | 112 | 52.2 |
| 0.019 | 180 | 51.1 |
| 0.019 | 273 | 50.3 |
| 0.019 | 378 | 49.2 |
| 0.019 | 464 | 49.2 |
| 0.019 | 551 | 48.0 |
| 0.019 | 638 | 47.3 |
| 0.019 | 724 | 46.5 |
| 0.019 | 1003 | 42.6 |
| 0.019 | 1102 | 42.3 |
| 0.019 | 1207 | 40.7 |
Data were digitized from Figs. 1 and 2 of the reference.