There was a problem with the connection!

NIST X-ray Photoelectron Spectroscopy Database (SRD 20), Version 5.0

Details Summary:


Tab Page Summary

General:
Tb/Fe/W
(sup 8)S7/2 multiplet
terbium/iron/tungsten
alloy, element

Citation:
Starke K., Baumgarten L., Arenholz E., Navas E., Kaindl G.
Phys. Rev. B 50, 1317
Pub Year:
1994

Data Processing:
Photoelectron Line

Measurement:
Anode Material:
other source
X-ray Energy:
48
Overall Energy Resolution (eV):
Calibration:
FL = Fermi level
Charge Reference:
Conductor
Energy Scale Evaluation:
Reliable (reported energy within 300 eV of a reference energy)
Comment:
2 ML Tb/10 ML Fe/W(110). The sample was annealed (T = 900 K, time = 10 min). The thickness was measured using a quartz-crystal thickness monitor. Using LEED, a cubic structure was observed, indicating TbFe2 formation.

Specimen:
Method of Determining Specimen Composition:
Method of Determining Specimen Crystallinity:
Low-energy Electron Diffraction
Specimen Temperature (K):
110